鋁型材表面油痕和水印避免!

來源:http://www.gdjsdtc.com/ 發布時間:2023-03-22

鋁型材表面油痕的特性反映:
The characteristics of oil marks on the surface of aluminum profiles reflect:
鋁型材時效前油漬不擦干凈在時效后在鋁材表面產生水印,氧化后呈暗斑且有高度。
The oil stains on the aluminum profile before aging are not wiped clean. After aging, watermarks are generated on the surface of the aluminum profile, and after oxidation, they appear as dark spots and have a height.
鋁型材表面油痕產生原因:
Reasons for oil marks on the surface of aluminum profiles:
1、成品鋸鋸切油漬留在鋁型材兩頭,搬(抬)料時手套不干凈甚至粘有石墨灰;
1. The oil stains left on both ends of the aluminum profile during the sawing and cutting of the finished product, and the gloves were not clean or even adhered with graphite dust when moving (lifting) the material;
2、鋁型材拉伸時手套臟拿料過長,鋸切未去掉;
2. When stretching aluminum profiles, the gloves are dirty and the material is taken too long, and the sawing is not removed;
3、中間理料時手套臟,留“印記”;
3. Gloves are dirty and leave "marks" during intermediate material handling;
4、擠壓設備工具漏滴油跡(行車,吊裝帶)。
4. The tools of the extrusion equipment leak oil stains (traveling crane, lifting belt).

鋁卷生產廠家
鋁型材表面油痕去除辦法:
Method for removing oil marks on the surface of aluminum profiles:
1、鋁材生產過程中理料,抬搬料時手套要干凈,有油跡要及時擦掉;
1. During the production process of aluminum materials, gloves should be clean when lifting and transporting materials, and any oil stains should be promptly wiped off;
2、拉伸鋁材時拿料要適當;
2. When stretching aluminum materials, take appropriate materials;
3、理料,抬搬料時的手套和拉伸拿料,加棒時的手套要分開;
3. Material handling, gloves for lifting and carrying materials, and gloves for stretching and taking materials, and gloves for adding rods should be separated;
4、設備,工具注意漏油,墊紙墊條吊帶等要干凈。
4. Attention shall be paid to oil leakage of equipment and tools, and the paper pad, strip sling, etc. shall be clean.
鋁型材表面水印的特性反映:
The characteristics of the watermark on the surface of aluminum profiles reflect:
鋁型材表面出現銀灰色濕狀印斑,鋁合金型材隨氧化堿洗的強度增加而減淡或消失。
Silver gray wet stains appear on the surface of aluminum profiles, and aluminum alloy profiles fade or disappear as the strength of oxidation and alkali washing increases.
鋁型材表面水印產生原因:
Reasons for generating watermarks on the surface of aluminum profiles:
鋁型材表面局部沾水淋雨,經型材表面淬火氧化層細微小孔滲入鋁基體,形成三羥鋁石,隨水份停留時間長短而現明淡,如果水中有雜質(鹽,亞硝酸等)會產生腐蝕斑。
Local parts of the surface of aluminum profiles are soaked in water and rain. After being quenched on the surface of the profile, the oxide layer penetrates into the aluminum matrix through fine pores, forming trihydroxyaluminite, which gradually fades with the length of the water retention time. If there are impurities (salt, nitric acid, etc.) in the water, corrosion spots will occur.
鋁型材表面水印去除辦法:
Method for removing watermarks on the surface of aluminum profiles:
沾水的鋁型材要馬上擦干,在時效前需要擦干,條件充許的話適當增加堿冼時間和氧化膜厚度。
Aluminum profiles that have been wetted with water should be wiped dry immediately and before aging. If conditions permit, the alkali washing time and oxide film thickness should be appropriately increased.

主站蜘蛛池模板: 久久久久亚洲av无码专区桃色| 曰韩内射六十七十老熟女影视| 又爽又黄又无遮挡网站动态图| 两口子交换真实刺激高潮| 女人脱了内裤趴开腿让男生摸| 国产日韩欧美| 国精产品自偷自偷综合下载 | 女人高潮被爽到呻吟在线观看| 日本欧美一区二区三区在线播放| 日日噜噜噜夜夜爽爽狠狠| 亚洲av无码一区二区三区在线播放| 国产精品 视频一区 二区三区| 无码人妻丰满熟妇区五十路| 天天躁夜夜踩很很踩2022| 国产三级av在线播放| 曰批免费视频播放免费| 永久免费av无码入口国语片| 八戒八戒午夜视频| 99re久久精品国产| 2018高清国产一区二区三区| 日韩日韩日韩日韩日韩| 久久免费观看午夜成人网站| 熟妇人妻无码中文字幕| 久久久久亚洲av无码麻豆| 国产成人精品一区二区三区无码| 国内精品久久久久久久小说 | 欧美最猛黑人xxxx黑人猛交| 中国精品18videosex性中国| 四虎成人精品一区二区免费网站| 亚洲欧洲日本综合aⅴ在线| 国产精品18久久久久久vr| 国产精品高潮呻吟av久久动漫| 无码熟妇人妻av在线网站| 国产产区一二三产区区别在线| 久久久精品国产sm调教网站| 肥臀熟女一区二区三区| 精品日产卡一卡二卡麻豆| 国产98色在线 | 日韩| 中文字幕一区二区三区乱码| 大雞巴亂倫有声小说| 国产成人无码一二三区视频|